Units
|
Test Method
|
Ultem 1000
|
|
Description
|
-
|
-
|
PolyEtherImide
|
|
Physical Properties
|
- |
- |
- |
|
Density
|
(lb/in3)
|
D792
|
0.046
|
|
-
|
(g/cm3)
|
D792
|
1.28
|
|
Water Absorption, 24 hrs
|
%
|
D570
|
0.25
|
|
Tensile Strength
|
psi
|
D638
|
16,500
|
|
Tensile Modulus
|
psi
|
D638
|
475,000
|
|
Tensile Elongation at break
|
%
|
D638
|
80
|
|
Flexural Strength
|
psi
|
D790
|
20,000
|
|
Fexural Modulus
|
psi
|
D790
|
500,000
|
|
Compressive Strength
|
psi
|
D695
|
22,000
|
|
Hardness
|
Rockwell M
|
D785
|
M112/R125
|
|
Izod Notched Impact
|
ft.- lb / in
|
D256
|
0.5
|
|
Dielectric Strength (short time, 1/8" thick)
|
V / mil
|
D149
|
830
|
|
Dielectric Constant at 1 MHz
|
-
|
5D150
|
3.15
|
|
Dissipation Factor at 1 MHz
|
-
|
D150
|
0.013
|
|
Volume Resistivity
|
Ohm-cm
|
D257
|
6.7 x 1017
|
| | | |
|
Thermal Properties
|
- |
- |
- |
|
Coefficient of Linear Thermal Expansion
|
in./in./°F
|
D696
|
3.1 x 10-5
|
|
Heat deflection temperature 264 psi
|
°F / °C
|
D648
|
392 / 200
|
|
Glass transition Temperature
|
°F / °C
|
D3418
|
419 / 215
|
|
Max Operating Temperature
|
°F / °C
|
-
|
340 / 171
|
|
Thermal Conductivity
|
BTU in. / ft2. hr2°F)
|
C177
|
0.90
|
|
Flammability Rating
|
-
|
UL94
|
V-O
|